Maighnéad Cast AlNiCo Airíonna Fisiceacha | |||||||||
Ábhar | Grád | Remanence | Temp.—Coeff. de Br | Comhéigeantacht | Temp.—Coeff. de Hcj | uas. Táirge Fuinnimh | uas. Teocht Oibriúcháin | Dlús | |
Br (KGs) | Hcb (TÚ) | (BH) max. (MGOe) | g/cm³ | ||||||
Isotrópach | LN9 | 6.8 | -0.03 | 0. 38 | -0.02 | 1.13 | 450 ℃ | 6.9 | |
Isotrópach | LN10 | 6.0 | -0.03 | 0. 50 | -0.02 | 1. 20 | 450 ℃ | 6.9 | |
Isotrópach | LNG12 | 7.2 | -0.03 | 0. 50 | +0.02 | 1.55 | 450 ℃ | 7.0 | |
Isotrópach | LNG13 | 7.0 | -0.03 | 0. 60 | +0.02 | 1. 60 | 450 ℃ | 7.0 | |
Isotrópach | LNGT18 | 5.8 | -0.025 | 1.25 | +0.02 | 2. 20 | 550 ℃ | 7.3 | |
Anisotrópach | LNG37 | 12.0 | -0.02 | 0. 60 | +0.02 | 1.65 | 525 ℃ | 7.3 | |
Anisotrópach | LNG40 | 12.5 | -0.02 | 0. 60 | +0.02 | 5.00 | 525 ℃ | 7.3 | |
Anisotrópach | LNG44 | 12.5 | -0.02 | 0.65 | +0.02 | 5.50 | 525 ℃ | 7.3 | |
Anisotrópach | LNG52 | 13.0 | -0.02 | 0. 70 | +0.02 | 6.50 | 525 ℃ | 7.3 | |
Anisotrópach | LNG60 | 13.5 | -0.02 | 0.74 | +0.02 | 7.50 | 525 ℃ | 7.3 | |
Anisotrópach | LNGT28 | 10.8 | -0.02 | 0.72 | +0.03 | 3. 50 | 525 ℃ | 7.3 | |
Anisotrópach | LNGT36J | 7.0 | -0.025 | 1.75 | +0.02 | 4.50 | 550 ℃ | 7.3 | |
Anisotrópach | LNGT32 | 8.0 | -0.025 | 1.25 | +0.02 | 4. 00 | 550 ℃ | 7.3 | |
Anisotrópach | LNGT40 | 8.0 | -0.025 | 1.38 | +0.02 | 5.00 | 550 ℃ | 7.3 | |
Anisotrópach | LNGT60 | 9.0 | -0.025 | 1.38 | +0.02 | 7.50 | 550 ℃ | 7.3 | |
Anisotrópach | LNGT72 | 10.5 | -0.025 | 1. 40 | +0.02 | 9.00 | 550 ℃ | 7.3 | |
Maighnéad AlNiCo sintered Airíonna Fisiceacha | |||||||||
Ábhar | Grád | Remanence | Temp.—Coeff. de Br | Comhéigeantacht | Comhéigeantacht | Temp.—Coeff. de Hcj | uas. Táirge Fuinnimh | uas. Teocht Oibriúcháin | Dlús |
Br (KGs) | Hcb (KA/m) | Hcj (KA/m) | (BH)uas. (KJ/m³) | g/cm³ | |||||
Isotrópach | SALNICO4/1 | 8.7-8.9 | -0.02 | 9-11 | 10-12 | -0.03~0.03 | 3.2-4.8 | 750 ℃ | 6.8 |
Isotrópach | SALNICO8/5 | 5.3-6.2 | -0.02 | 45-50 | 47-52 | -0.03~0.03 | 8.5-9.5 | 750 ℃ | 6.8 |
Isotrópach | SALNICO10/5 | 6.3-7.0 | -0.02 | 48-56 | 50-58 | -0.03~0.03 | 9.5-11.0 | 780 ℃ | 6.8 |
Isotrópach | SALNICO12/5 | 7.0-7.5 | -0.02 | 50-56 | 53-58 | -0.03~0.03 | 11.0-13.0 | 800 ℃ | 7 |
Isotrópach | SALNICO14/5 | 7.3-8.0 | -0.02 | 47-50 | 50-53 | -0.03~0.03 | 13.0-15.0 | 790 ℃ | 7.1 |
Isotrópach | SALNICO 14/6 | 6.2-8.1 | -0.02 | 56-64 | 58-66 | -0.03~0.03 | 14.0-16.0 | 790 ℃ | 7.1 |
Isotrópach | SALNICO14/8 | 5.5-6.1 | -0.01 | 75-88 | 80-92 | -0.03~0.03 | 14.0-16.0 | 850 ℃ | 7.1 |
Isotrópach | SALNICO18/10 | 5.7-6.2 | -0.01 | 92-100 | 99-107 | -0.03~0.03 | 16.0-19.0 | 860 ℃ | 7.2 |
Anisotrópach | SALNICO35/5 | 11-12 | -0.02 | 48-52 | 50-54 | -0.03~0.03 | 35.0-39.0 | 850 ℃ | 7.2 |
Anisotrópach | SALNICO29/6 | 9.7-10.9 | -0.02 | 58-64 | 60-66 | -0.03~0.03 | 29.0-33.0 | 860 ℃ | 7.2 |
Anisotrópach | SALNICO32/10 | 7.7-8.7 | -0.01 | 90-104 | 94-109 | -0.03~0.03 | 33.0-38.0 | 860 ℃ | 7.2 |
Anisotrópach | SALNICO33/11 | 7.0-8.0 | -0.01 | 107-115 | 111-119 | -0.03~0.03 | 33.0-38.0 | 860 ℃ | 7.2 |
Anisotrópach | SALNICO39/12 | 8.3-9.0 | -0.01 | 115-123 | 119-127 | -0.03~0.03 | 39.0-43.0 | 860 ℃ | 7.25 |
Anisotrópach | SALNICO44/12 | 9.0-9.5 | -0.01 | 119-127 | 124-132 | -0.03~0.03 | 44.0-48.0 | 860 ℃ | 7.25 |
Anisotrópach | SALNICO37/15 | 7.0-8.0 | -0.1 | 143-151 | 150-158 | -0.03~0.03 | 37.0-41.0 | 870 ℃ | 7.2 |
Nóta: · Fanfaimid mar a chéile thuas mura sonraítear ón gcustaiméir. Tá teocht agus comhéifeacht teocht Curie le haghaidh tagartha amháin, ní mar bhunús le cinneadh. · Is féidir uasteocht oibre maighnéad a athrú mar gheall ar chóimheas faid agus trastomhais agus fachtóirí timpeallachta. |
Gné:
1. Tá ionduchtú ard iarsma ag maighnéad AlNiCo ach coercivity íseal. Oibríonn sé cobhsaí ag teocht mhór, ag cothabháil a saintréithe maighnéadacha idir
–250ºC agus 550ºC. Bunaithe ar ionduchtú maighnéadach níos fearr, úsáidtear é den chuid is mó i dtrealamh tomhais agus córais braite.
2. Is ábhar leochaileach é Alnico agus ní féidir é a athrú ach amháin le linn an phróisis réitigh. Treoshuíomh sé bainte amach le linn cóireála teasa, a tháirgeadh réimse maighnéadach
leis an treo maighnéadaithe sainithe.
3. Mar gheall ar an bhfórsa coercive íseal, is féidir tionchar a imirt go héasca ar mhaighnéid AlNiCo le fórsa maighnéadach droim ar ais agus tionchar iarainn. Sin an fáth gur féidir iad a dhímagnetú go héasca
ag tionchair sheachtracha. Ar an gcúis seo, níor chóir maighnéid AlNiCo a stóráil agus a phacáil leis na cuaillí céanna atá i gcoinne a chéile.
4. I gciorcad oscailte, ba chóir go mbeadh an cóimheas faid/trastomhas (L/D) ar a laghad 4:1. Le fad níos giorra
5. Iompraíonn maighnéid AlNiCo go maith i gcoinne ocsaídiúcháin. Níl aon sciath ag teastáil le haghaidh cosaint dromchla.
Feidhmchláir:
Úsáid i dtáirgí ard-íogaireachta mar Ionstraimí, Méadair, Fóin Póca, páirteanna Gluaisteán. Feistí leictreafhuaimiúla, Mótair, Teagaisc agus Aeraspáis
míleata, etc.
Socraíodh na luachanna sonraithe go léir ag baint úsáide as samplaí caighdeánacha de réir IEC 60404-5. Feidhmíonn na sonraíochtaí seo a leanas mar luachanna tagartha agus féadfaidh siad a bheith éagsúil.